TC500系列儀器質(zhì)量、性能、工藝滿足您對(duì)金屬、難熔物、其他無(wú)機(jī)材料日常生產(chǎn)中氮/氧分析的需要

Determination of Oxygen and Nitrogen in
Reactive/Refractory Metals and Their Alloys*
 
Approval
ASTM E-1409 Oxygen Determination in Titanium and Titanium Alloys
ASTM E-1569 Oxygen Determination in Tantalum
ASTM E-1937 Nitrogen Determination in Titanium and Titanium Alloys
 
Sample Preparation
A clean representative sample is required in order to obtain optimum results. Solid samples can be leached in suitable acid or abraded with a clean file, rinsed in acetone, and dried with warm air. Refer to ASTM methods above for further details.
 
Accessories
782-720 Crucible; 782-721 Electrode Tip; 502-344 UHP Nickel
Baskets; 501-073 Graphite; 503-032 Glass Accelerator Scoop;
501-059 Tin Capsules—for powdered samples. (Additional steps required for powdered samples are noted in parenthesis.)
 
Calibration Standard
LECO 501-320 Titanium Pin, 502-047 Zirconium Pin, NIST, or other suitable reactive/refractory metal standard.
 
Method Parameters
Analysis Parameters
Outgas Cycles                           2
Analysis Delay (seconds)             20
Analysis Comparator                 1
Analysis Type                              Auto
 
Element Parameters                  Oxygen           Nitrogen
Minimum Time (seconds)
35
55
Integration Delay (seconds)
5
15
Comparator Level (%)
1
1
 
Furnace Parameters
Furnace Control Mode             Power
Purge Time (seconds)                    15
Outgas Time (seconds)                20
Cool Time (seconds)                    5
Outgas Power (Watts)                 6300
Analyze Power (Watts)                5300
 
 
 
 
 


 

*This includes Ti, Zr, W, Mo, Ta, Nb, Hf, and their alloys.

 
TC500


 

 
Typical Results
 
 
 
Titanium Pin
Mass (g)
Oxygen (%)
Nitrogen (%)
 
0.1135
0.1808
0.0189
 
0.1133
0.1843
0.0194
 
0.1134
0.1831
0.0184
 
0.1138
0.1819
0.0188
 
0.1133
0.1821
0.0195
 
0.1131
0.1829
0.0185
 
0.1134
0.1833
0.0191
 
0.1143
0.1849
0.0194
 
0.1125
0.1837
0.0189
 
0.1072
0.1830
0.0191
 
Average
0.1830
0.0190
 
Std. Dev.
0.0012
0.0004
 
Zirconium Wire
 
Mass (g)
 
Oxygen (%)
 
Nitrogen (%)
 
0.1067
0.1246
0.0017
 
0.0978
0.1273
0.0017
 
0.1180
0.1246
0.0019
 
0.1097
0.1235
0.0014
 
0.1141
0.1272
0.0017
 
0.1017
0.1226
0.0018
 
0.1140
0.1269
0.0020
 
0.0987
0.1239
0.0020
 
0.1015
0.1233
0.0022
 
0.1197
0.1270
0.0020
 
Average
0.1251
0.0018
 
Std. Dev.
0.0018
0.0002
 
Procedure
 
 
 
1.   Determine the blank as follows:
a.   Enter the "blank" ID code with a 1.0000 g weight in the weight stack.
b.   Press the loader control switch, the sample loader will open.
c.   Place one 502-344 UHP Nickel basket into the loading head using clean tweezers.
(Place a 501-059 Tin capsule into the Nickel basket before placing it in the loading head.)
d.   Press the loader control switch, the sample loader will close and seal and the furnace electrode will open.
e.   Remove crucible from electrode tip and discard.  Clean furnace area using the appropriate brushes.  Vacuum away loose dust.
f.    Place ~0.05 g 501-073 into the bottom of a 782-720 crucible.  ~0.05 g is approximay a ¼ full
503-032 glass accelerator scoop.
g.   Place the crucible on the lower electrode.
h.   Press the loader control switch, the furnace electrode will close and the analysis sequence will start automatically.
i.    Repeat steps 1a through 1h at least four more times.
j.    Enter blank following routine outlined in operator's instruction manual.
2.   Calibrate the instrument as follows:
a.   Weigh the calibration sample. (Weigh the calibration sample into the tin capsule.)
b.   Enter the calibration sample ID code and sample weight in the weight stack.
c.   Place the calibration sample (capsule) into a nickel basket.
d.   Press the loader control switch, the sample loader will open.
e.   Carefully place the calibration sample/nickel basket (capsule) into the loading head using clean tweezers.  Make sure that the calibration sample (capsule) stays in the basket and the basket
stays upright.
f.    Press the loader control switch, the sample loader will close and seal and the furnace electrode will open.
continued on page 3


 

Procedure (continued from page 2)
g.   Remove crucible from electrode tip and discard.  Clean furnace area using the appropriate brushes.  Vacuum away loose dust.
h.   Place ~0.05 g graphite into the bottom of a crucible.
i.    Place the crucible on the lower electrode.
j.    Press the loader control switch, the furnace electrode will close and the analysis sequence will start automatically.
k.   Repeat steps 2a through 2j a minimum of three times.
l.    Complete a calibration by following the auto calibration procedure as outlined in the operator's instruction manual.
m.  Verify the calibration by analyzing the calibration sample again.  It should fall within the expected tolerances.  If not, repeat steps 2a through 2l again.
3.   Analyze the samples as follows:
a.   Weigh ~0.1 g sample. (Weigh the sample into the tin capsule.)
b.   Enter the sample ID code and sample weight in the weight stack.
c.   Place the sample (capsule) into a nickel basket.
d.   Press the loader control switch, the sample loader will open.
e.   Carefully place the sample/nickel basket (capsule) into the loading head using clean tweezers.
Make sure that the sample (capsule) stays in the basket and the basket stays upright.
f.    Press the loader control switch, the sample loader will close and seal and the furnace electrode will open.
g.   Remove crucible from electrode tip and discard.  Clean furnace area using the appropriate brushes.  Vacuum away loose dust.
h.   Place ~0.05 g graphite into the bottom of a crucible.
i.    Place the crucible on the lower electrode.
j.    Press the loader control switch, the furnace electrode will close and the analysis sequence will start automatically.
 
Theory of Operation
The TC500 is a microprocessor-based, software-controlled instrument that measures both nitrogen and oxygen in a wide variety of metals, refractories, and inorganic materials. The inert gas fusion principle is employed. A weighed sample, placed in a high-purity graphite crucible, is fused under a flowing helium gas stream at temperatures sufficient to release oxygen, nitrogen, and hydrogen. The oxygen in the
sample, combines with the carbon from the crucible to form carbon monoxide. The nitrogen present in
the sample releases as molecular nitrogen, and any hydrogen present is released as hydrogen gas. The helium carries the sample gases through heated rare earth copper oxide which converts carbon
monoxide to carbon dioxide (CO2) and hydrogen to water (H2O). The nitrogen passes through
unchanged. The gases are then passed through a CO2  infrared (IR) cell where the oxygen is measured as
CO2. CO2  and H2O are then removed by a Lecosorb/Anhydrone trap, while the nitrogen passes through
to a thermal conductivity (TC) cell for determination.


 

TC500 Flow Diagram
 
 
 
 
 

留言框

  • 產(chǎn)品:

  • 您的單位:

  • 您的姓名:

  • 聯(lián)系電話:

  • 常用郵箱:

  • 省份:

  • 詳細(xì)地址:

  • 補(bǔ)充說(shuō)明:

  • 驗(yàn)證碼:

    請(qǐng)輸入計(jì)算結(jié)果(填寫阿拉伯?dāng)?shù)字),如:三加四=7
技術(shù)支持:化工儀器網(wǎng)   sitemap.xml   管理登陸
©2024 版權(quán)所有:寧波市鄞州瑾瑞儀器設(shè)備有限公司   備案號(hào):浙ICP備14028217號(hào)-3

浙公網(wǎng)安備33020402000311號(hào)

99香蕉国产精品偷在线观看| 他跨越山海而来| 国产乱码精品一区二区三区中文| 太深太粗太爽太猛了视频免费观看| 亚洲精品一二三区尤物tv| 我要受不了了快添我的奶头| 强壮公弄得我次次高潮厨房| 奶头被教练摸得受不了| 韩国精品无码少妇在线观看 | 三男一女做2爱A片免费视频| 无码丰满熟妇juliaann与黑人| 极品教师在线观看免费完整版| 男人放进女人阳道视频观看| 欧美18videosex性欧美| 大炕上的性满足| 国产精品18久久久久久vr| 级毛片内射视频| 午夜时刻免费入口| 一人观看的电影免费观看| 欧美亚洲一区二区三区| 野外真人实战cs| 欧美粗大猛烈18p| 性色AV一区二区三区咪爱四虎| 国产成人精品白浆久久69| 超清中文乱码字幕在线观看| 亚洲精品一区二区久久| 少妇被又大又粗又爽毛片欧美| 双性人妖互交videos| 欧美xxxx黑人又粗又长精品| 污污污污污污www网站免费| 疯狂的交换1—6大团结| 乱妇乱女熟妇熟女网站| 女高中生自慰污污网站| 道具play震动按摩器| 免费视频网站在线看视频| 强奷漂亮少妇高潮a片xxxx| 去部队探亲被全队肉辣文| 精品国产18久久久久久| 美男被强行糟蹋np各种play| 公车上拨开丁字裤进入电影| 欧美性大战xxxxx久久久|